Material scienceMarch 1, 202615 min read

Can copper and aluminium touch? Galvanic corrosion

Galvanic corrosion, also called contact or bimetallic corrosion, starts when two different metals touch in the presence of moisture: the less noble one dissolves. In electrical work the pair is almost always copper and aluminium. This page gives the real voltage between them and what each published figure means, shows which other metals aluminium can safely touch, and explains how a bimetal transition removes the problem.

In short

Copper and aluminium can touch, but where moisture reaches the joint the aluminium corrodes. In the MIL-DTL-14072F galvanic table the two metals sit 0.55 V apart, more than twice the 0.25 V that specification allows between metals in contact. The permanent fix is a bimetal transition, so that copper touches only copper and aluminium only aluminium.

0.55V
Cu-Al gap, MIL-DTL-14072F
0.25V
Max. gap allowed between metals in contact
0.15V
Guidance for marine and outdoor air
M6–M20
Bimetallic washers from stock

What CUPAL® is, in one line: a roll-bonded copper-aluminium bimetal, a copper layer bonded onto an aluminium layer across the whole face, about 30 % copper by layer thickness. It is not copper-clad aluminium (CCA) wire, in which a thin copper skin covers an aluminium core.

Facing this joint right now?

Tell us what meets what (a copper lug on an aluminium busbar, a cable on a mast, bar to bar), plus the bolt size and how many you need. We come back with the transition that fits and a price within 24 hours. Washers ship from stock in 2–10 working days; cut-to-size parts take 5–10 working days in production.

Send us the joint, get a quote in 24 hours →

What is galvanic corrosion?

Galvanic corrosion is an electrochemical process. Two dissimilar metals in electrical contact, bridged by an electrolyte such as condensation, humid air or salt spray, form a cell: the potential difference between them drives a current, and the less noble metal, the anode, gradually dissolves.

Three conditions have to be met at once: two different metals in contact, an electrolyte connecting them, and a potential difference large enough to drive the current. Remove any one and the corrosion stops. A bimetal transition removes the first: at the bolted faces each metal only ever touches its own kind, and the copper-aluminium interface sits sealed inside the material.

How big is the copper-aluminium potential difference?

Four different numbers circulate for this pair, and they measure different things. Only one of them describes a real joint.

FigureCopperAluminiumGapWhat it describes
Standard electrode potential, vs SHE (CRC Handbook)+0.34 V−1.66 V≈ 2.0 VBare metal in a solution of its own ions. A thermodynamic bound, not a joint
Galvanic series in seawater, vs saturated calomel electrode (MIL-DTL-14072F, Table VI)−0.20 V−0.75 V0.55 VMeasured on real alloys in seawater at room temperature. The practical figure
Anodic index (same table, re-zeroed on gold)0.35 V0.90 V0.55 VThe scale design limits are written in
Contact (Volta) potential, from work functions (CRC Handbook)4.53–5.10 eV4.06–4.26 eV≈ 0.3–1 VThe potential across a dry metal-to-metal contact. No current flows

The figure to use is 0.55 V. It comes from MIL-DTL-14072F, a US military specification for finishing electronic equipment. Its Table VI groups metals by their potential against a saturated calomel electrode in seawater at room temperature and derives an anodic index from it. Aluminium here means wrought alloys outside the 2000 series, which covers busbar grades and CUPAL's own EN AW-1050A. The same table sets the rule: metals in contact should be no more than 0.25 V apart. Copper and aluminium are more than twice that. Common engineering guidance tightens the limit to 0.15 V for harsh conditions such as marine or outdoor air and relaxes it to 0.50 V for temperature- and humidity-controlled rooms. Copper-aluminium fails even the relaxed figure.

The roughly 2 V gap between the textbook standard potentials is correct thermodynamics but the wrong number for a joint. It describes bare metal in a solution of its own ions. Aluminium in air is always covered by an oxide film, which puts its working potential far above −1.66 V. Use the 2 V to explain why aluminium is the anode, not to size the risk.

Contact potential is not galvanic potential

Searches for the "contact potential difference" between aluminium and copper usually want one of the figures above, but in physics the term means something else. When two metals touch, electrons flow from the one with the lower work function (aluminium) to the one with the higher (copper) until their Fermi levels line up. What remains is a contact, or Volta, potential equal to the work-function difference: with CRC Handbook values of 4.06–4.26 eV for aluminium and 4.53–5.10 eV for copper, roughly 0.3 to 1 V depending on crystal face and surface state. It exists in a perfectly dry joint, no current flows, and on its own it corrodes nothing. Corrosion needs the galvanic couple, and the galvanic couple needs an electrolyte.

Why is the copper-aluminium combination particularly dangerous?

Copper lugs land on aluminium busbars, aluminium cables land on copper terminals, and copper bonding conductors are bolted to aluminium structures every day. Four things make this pairing dangerous.

1. The gap is large

At 0.55 V the copper-aluminium gap is more than twice the 0.25 V allowed between metals in contact. MIL-DTL-14072F adds a second warning: when the cathodic part is much larger than the anodic one, the attack on the anode is concentrated. An aluminium lug on a large copper busbar is that unfavourable case.

2. Moisture is almost always present

Switchgear, distribution boards and outdoor installations nearly always see moisture, as condensation or as humidity in the air. That is the electrolyte the cell needs.

3. The aluminium oxide grows

As the aluminium surface corrodes it forms aluminium oxide, an electrical insulator, and the joint's contact resistance rises.

4. Bolted joints loosen

Aluminium oxide takes up more volume than the metal it came from, which physically loosens bolted joints.

A specific case: copper cable to an aluminium mast

The joint behind many of the questions we receive is a copper bonding, earthing or lightning conductor bolted to an aluminium mast: on a sailing yacht, an antenna or telecom mast, or a wind-turbine tower. Salt spray is the harshest electrolyte this joint meets, and the 0.55 V copper-aluminium gap is almost four times the 0.15 V guidance for marine air.

Tinned marine cable does not change the verdict. Tin-plated parts sit at 0.60 V in the same table, still 0.30 V from aluminium, and wherever the tin is worn or scratched the copper underneath is back in contact. A stainless washer does not help either, for the reason in the table below. Copper bonding to aluminium masts covers what fails on a mast and which bimetal part to fit.

Galvanic corrosion of aluminium: which metals it can touch

The question behind most searches on aluminium galvanic corrosion is simply which metals may touch it. The anodic index answers it directly. Values from MIL-DTL-14072F, Table VI; wrought aluminium (all series except 2000) is 0.90 V.

Metal touching aluminiumAnodic indexGap to aluminiumWhich metal corrodesWithin 0.25 V?
Copper, low brasses and bronzes; austenitic stainless steel (A2, A4)0.35 V0.55 VAluminiumNo, not even within 0.50 V
Yellow brass and bronzes0.40 V0.50 VAluminiumNo
18 % chromium (ferritic) stainless steel0.50 V0.40 VAluminiumNo
Tin-plated parts0.60 V0.30 VAluminiumNo
Tin plate, tin-lead solder0.65 V0.25 VAluminiumAt the limit
Hot-dip galvanised steel1.20 V0.30 VZincNo, and here the zinc corrodes
Other wrought aluminium0.90 V0NeitherYes

Two rows matter most in electrical work. Austenitic stainless steel, the A2 and A4 grades used for stainless fasteners, sits in the same group as copper, so a stainless washer between a copper lug and an aluminium bar leaves the 0.55 V gap where it was and adds a third metal. And zinc reverses the roles: against galvanised steel it is the zinc, not the aluminium, that corrodes.

Real-world consequences

Rising contact resistance

The oxide layer and the corrosion products raise contact resistance. The joint heats up, and the heat speeds up the corrosion: a self-sustaining cycle.

Overheating and fire risk

Higher contact resistance generates heat, and in high-current joints the temperature can reach fire-hazard levels. The best-documented evidence comes from aluminium house wiring. A survey for the US Consumer Product Safety Commission found that homes wired with aluminium before 1972 were 55 times more likely than copper-wired homes to have at least one outlet connection reach "fire hazard conditions" (CPSC Publication 516). The failures were at the connections, where resistance rose until the joint overheated.

Failure and outages

Loose, corroded joints fail over time: intermittent contact, arcing, and eventually a full outage.

How does CUPAL solve the problem?

CUPAL bimetal contains copper and aluminium in one part: an EN AW-1050A aluminium layer cold-roll-bonded to a Cu-ETP copper layer, inseparably. It deals with the galvanic couple on three levels.

1. Same metal meets same metal

A CUPAL washer or transition part sits between the copper and the aluminium conductor so that each face meets its own metal:

  • the copper face against the copper lug, bar or terminal
  • the aluminium face against the aluminium busbar, lug or structure

Both outer contacts are like-metal contacts, with no potential difference across them. The same washer serves a copper lug on an aluminium bar and an aluminium lug on a copper bar; only the orientation changes.

2. The copper-aluminium interface is inside the part

The copper-aluminium boundary lies inside the material, metallurgically bonded, where the contact faces do not expose it to moisture. Only at the rim of a washer or the cut edge of a part does the bond line reach the surface. That is why outdoor, damp or salt-laden joints need that edge protected or covered. Tell us the conditions when you ask for a quote and we will say what the joint needs.

3. Low, stable contact resistance

Both bolted interfaces are like-metal contacts, so the joint behaves like an ordinary copper-copper or aluminium-aluminium bolted joint. Its contact resistance does not climb the way a direct copper-aluminium contact does.

Which CUPAL part for which joint

Bimetallic washers

The most common case: a bimetallic washer M6–M20 between a copper cable lug and an aluminium busbar, or the same washer turned over under an aluminium lug on a copper bar. Fitting takes minutes; surface preparation, orientation and edge protection are in the installation guide.

Bimetal cable lugs

Where an aluminium cable still has to be terminated on a copper terminal, a bimetal cable lug puts the transition inside the lug itself.

CUPAL strip

Where the transition has to bend or wrap around a connection point, as in lightning protection, CUPAL strip is the same bimetal in band form.

Plates and parts cut to a drawing

For whole busbar faces, use CUPAL bimetal plates or a part cut to your drawing from CUPAL sheet; the minimum is one 500 × 500 mm sheet. Which of these forms belongs in a given joint, and when a crimped bimetal lug or inline connector replaces all of them, is worked through joint by joint in connecting copper to aluminium.

Prevention or after the fact?

Preventing galvanic corrosion is always cheaper and simpler than repairing it. A bimetallic washer costs a fraction of replacing a failed joint, refurbishing switchgear or, at worst, covering fire damage.

Standards set requirements for the installed joint, not for a washer: IEC 61439 sets temperature-rise limits for low-voltage switchgear assemblies, IEC 61238 tests connectors for power cables, and DIN 43671 (copper) and DIN 43670 (aluminium) rate busbars for continuous current. No transition part is "certified" to them on its own. A bimetal transition is how a copper-aluminium joint is built so that it can meet them.


Questions about a specific joint? Send us the details and you get a priced answer within 24 hours.

Frequently asked questions

They can touch, but they should not share a joint that moisture can reach. With an electrolyte present (condensation, humid air or salt spray) the pair forms a galvanic cell and the aluminium corrodes. The two metals are 0.55 V apart in the MIL-DTL-14072F galvanic table, more than twice the 0.25 V that specification allows between metals in contact. The fix is a bimetal transition, so each metal touches only its own kind.
They form a galvanic cell. Wherever moisture, condensation or salt bridges the joint, the aluminium becomes the anode and corrodes, driven by a practical potential difference of about 0.55 V. The corrosion product is aluminium oxide, a poor conductor, so contact resistance climbs, the joint heats under load and the heat speeds up the corrosion. The oxide also takes up more volume than the metal, which loosens bolted joints.
Not on its own. Dry, solid copper and aluminium do not react with each other. Add an electrolyte, from condensation to salt spray, and they form a galvanic cell in which the aluminium dissolves. Copper that is already dissolved does react with aluminium directly: aluminium displaces copper from its salts.
Not in direct contact. MIL-DTL-14072F treats metals as compatible when they are within 0.25 V of each other; copper and wrought aluminium are 0.55 V apart, which also exceeds the 0.50 V that engineering guidance tolerates in climate-controlled rooms. Through a bimetal transition, where copper meets copper and aluminium meets aluminium, they work together without corroding.
It depends which potential you mean. For corrosion the useful figure is the galvanic one: 0.55 V in seawater per MIL-DTL-14072F (anodic index copper 0.35 V, aluminium 0.90 V). The textbook gap between standard electrode potentials, +0.34 V for copper and −1.66 V for aluminium, is about 2 V, but it describes bare metal in its own ion solution and overstates a real joint. The contact (Volta) potential of physics comes from the work functions (aluminium 4.06–4.26 eV, copper 4.53–5.10 eV, CRC Handbook), is roughly 0.3–1 V, and drives no current in a dry joint.
Only while it stays dry, and that is hard to guarantee. Without an electrolyte no galvanic current flows. But the 0.55 V gap exceeds even the 0.50 V that engineering guidance accepts for temperature- and humidity-controlled rooms, and condensation in switchgear is common. If the joint has to last without inspection, put a bimetal transition in it.
Copper corrodes aluminium. Aluminium is the less noble metal in any aluminium-copper pair, so it is the side that dissolves, and the damage shows on the busbar, the mast or the terminal rather than on the copper. Attack is concentrated where a small aluminium part sits on a large copper surface, such as an aluminium lug on a copper busbar. Protecting the joint means separating the metals, not coating the copper.
No. The A2 and A4 austenitic stainless steels used for stainless fasteners sit in the same MIL-DTL-14072F group as copper, 0.55 V from aluminium. A stainless washer between a copper lug and an aluminium bar keeps the same couple and adds a third metal to the joint. A bimetal washer removes the couple, because each of its faces meets its own metal.
By ending the direct dissimilar-metal contact. A CUPAL bimetal transition (washer, strip or plate) goes between the conductors so that the copper face meets the copper and the aluminium face meets the aluminium. Both contacts are like-metal, so there is no potential difference across them. The Cu/Al interface stays inside the part; only its rim shows the bond line, which is why outdoor and damp joints need that edge protected or covered.
Do not bolt them together directly. Put a copper-aluminium bimetal transition between them: a CUPAL washer for a single bolted lug, or a cut CUPAL plate where a whole busbar face meets copper. The aluminium side faces the aluminium busbar and the copper side faces the copper lug, so the dissimilar pair is never in contact at the joint face. Antioxidant paste slows the reaction but does not remove the couple, and it needs re-inspection; the bimetal transition is permanent.
Corrosion forms an insulating aluminium-oxide layer that raises the joint's contact resistance. The higher resistance generates heat, the heat speeds up the corrosion, and the joint heats and loosens. In high-current applications the temperature rise can reach fire-hazard levels, leading to intermittent contact, arcing and eventually an outage.
They set requirements for the installed joint, not for the transition part. IEC 61439 sets temperature-rise limits for low-voltage switchgear assemblies, IEC 61238 tests connectors for power cables, and DIN 43671 (copper) and DIN 43670 (aluminium) rate busbars for continuous current. No washer is certified to them on its own; a bimetal transition is how a copper-aluminium joint is built so that it can meet them.

Have a question?

Email us or use the form: we reply within 24 hours on working days.